焊槍故障Welding torch fault
1.焊槍未能正常引弧焊接,如果5秒鐘內(nèi)不能引燃,操作工應(yīng)按急停按鈕,立即查明原因。
If the welding torch can not fire within 5s,it should be cut off the button and checked the reason.
2. 造成的原因有可能有:焊機(jī)未開(kāi);鎢極與帶材距離過(guò)大;鎢極易氧化,帶材表面過(guò)臟或氧化層過(guò)厚。
Reasons:The welder is cut off;The distance of tungsten electrode and strip is too large;The tungsten electrode is easy oxidation;The strip surface is dirty and the oxidation is too thick.
3.故障排除后,重新引弧啟動(dòng)。
It can be welding after troubleshooting.
安全警告Warning
1.設(shè)備安裝斷電保護(hù)裝置
Power off for installation
2. 機(jī)器在運(yùn)作是,嚴(yán)禁靠近焊接機(jī)
Keep off the welder during running.
3.在焊接過(guò)程中,工作人員一定要有保護(hù)措施,如佩戴焊接防護(hù)眼鏡或面罩來(lái)保護(hù)眼睛和臉部,穿阻燃工作服等保護(hù)措施。
The staff must have protective measures, such as wear welding goggles ,take face mask to protect eyes and face, wear protection working clothes and so on.
焊接速度參數(shù)僅做參考Welding speed(just for reference)
板厚度Panel thickness(mm) |
電流Current(A) |
氣體壓力Air pressure |
焊槍速度Welding torch speed |
鎢極直徑Tungsten electrode diameter(mm) |
0.5 |
60-80 |
3--5 |
15--6 |
1.6 |
1.0 |
80-100 |
4--6 |
14--5 |
2.0 |
2.0 |
100-140 |
5--7 |
13--4 |
2.4 |
3.0 |
120-400 |
6--8 |
12--4 |
3.0 |